LiTaO3 exhibits excellent electro-optical,
piezoelectric and pyroelectric proerties. It has been widely used
for E-O devices, due to its good optical, NLO and E-O properties,
and higher damage threshold. U-Optics supplies high quality LiTaO3
boules and wafers with the following specifications for standard
applications. It may also offer other specifications upon request.
|
|
Standard Specifications of LiTaO3:
| Cut Type |
Vs (m/s) |
K2s (%) |
TCV (10-6/oC) |
TCD (10-6/oC) |
| X-112o Y |
3295 |
0.75 |
-16.50 |
22.3 |
| Y-Z |
3230 |
0.66 |
- |
35 |
Typical Diameter |
Diameter 3.0" ¡À 2mm |
Diameter 4.0" ¡À 2mm |
Typical Length |
¡Ü 120mm |
¡Ü 100mm |
Cut Type |
36¡ã Y, 42¡ã Y |
Main Parameters:
Transparency Range: |
400 - 5000nm |
Crystal Structure: |
Trigonal, Space group R3c,
Point group 3m |
Cell Parameters: |
a = 0.5154nm, c = 1.3783nm |
Mohs hardness: |
5.5 mohs |
Melting Point: |
1650 |
Curie Temperature: |
607 |
Density: |
7.46 g/cm3 |
Dielectric Constant: |
¦Î11/¦Î0 = 51.7, ¦Î33/¦Î0
= 44.5 |
Elastic Stiffness Coefficient: |
CE11 = 2.33(x
1011 N/m2) / CE33 = 2.77(x
1011 N/m2) |
Piezoelectric Strain Constant: |
d22 = 2.4 (x 10-11 C/N) / d33
= 0.8 (x 10-11 C/N) |
Electro-optical coefficients: |
r33 = 30.4pm/V |
Refractive index at 632.8nm: |
no = 2.176, ne
= 2.180 |
|